5.
Sprue, invest, and cast all sections
simultaneously in the alloy of choice. Do not use a carbon containing
investment. Burnout at 1700F degrees with a one hour heat soak.
When using a high palladium alloy, be careful not to overheat the alloy.
Use an oxygen setting of 10psi when torch melting.
Leave the casting attached to the casting button.
Immerse the castings in a rust-removing solution such as liquid wrench for
ten minutes.
Use the precision slotted Center Punch to separate the
male from the female. The precision slotted tip of the punch fits over
the bottom of the male attachment.
The FR center punch should be adjusted to medium
action. |